Asian Pacific Journal of Dentistry
Online ISSN : 2185-3487
Print ISSN : 2185-3479
Effect of low-pressure plasma treatment on the adhesion of poly (etheretherketone)
Riho Ito, Shojiro Shimizu , Motohiro Uo, Hiroshi Tsuchiyama, Masaomi Ikeda, Michael F Burrow, Toru Nikaido, Katsushi Okuyama
著者情報
ジャーナル オープンアクセス HTML 早期公開

論文ID: 25-0012

詳細
Abstract

Purpose: The use of computer-aided design and computer-aided manufacturing (CAD-CAM) systems has increased the need for reliable metal-free restorative materials. Poly (etheretherketone) (PEEK) shows excellent physical and mechanical properties, but its bonding protocols remain insufficiently established. Various surface treatments have been proposed to improve adhesion. This study investigated the effect of low-pressure plasma treatment on PEEK surfaces and evaluated the bond strength of a methyl methacrylate (MMA)-based adhesive applied to plasma-treated PEEK.

Methods: PEEK blocks were sectioned, sandblasted with 50 µm alumina particles, and divided into non-plasma-treated (PI[−]) and plasma-treated (PI[+]) groups. Each group was further classified by whether the adhesive was light-cured for 10 s or chemically cured. Specimens were bonded to steel rods with a dual-cure resin cement and stored in water at 37°C for 24 h. Groups were tested after either 0 or 5,000 thermal cycling (TC; 5-55°C). Tensile bond strength (TBS) was measured (n = 10), failure modes were analyzed by scanning electron microscopy, and surface wettability was evaluated by contact angle.

Results: A significant interaction between plasma and curing mode was observed (P < 0.05), whereas neither the interactions between plasma and TC nor between curing mode and TC were statistically significant (P > 0.05). Plasma treatment significantly reduced the contact angle (P < 0.05), indicating improved wettability.

Conclusion: Low-pressure plasma treatment enhanced the hydrophilicity of PEEK but did not improve bond strength. Light curing of the MMA-based adhesive significantly increased bond strength, suggesting improved bonding under light curing conditions.

Introduction

Recent developments in computer-aided design and computer-aided manufacturing (CAD-CAM) systems have greatly improved the accuracy, efficiency and consistency of inlay/crown restoration manufacture [1,2,3]. Consequently, the development of new dental materials compatible with CAD-CAM technology and suitable for efficient machining has been actively pursued. Along with these technological advances, the range of materials that can be processed using CAD-CAM systems has expanded, thereby broadening the scope of dental treatments and clinical applications.

Among these materials, poly (etheretherketone) (PEEK) is known for its excellent mechanical properties, chemical resistance and biocompatibility [4]. Due to these advantages, PEEK has been actively investigated and applied in dental research and clinical practice [5,6,7,8,9,10]. However, the molecular structure of PEEK is characterized by benzene rings connected via ketone and ether bonds, resulting in a low concentration of polar functional groups on its surface. This chemical property limits the effectiveness of conventional adhesive pretreatments with a functional monomer, thus presenting a considerable challenge for bonding to PEEK in dental applications [11,12]. To ensure the long-term functionality of PEEK-based restorations in the oral environment, the development of novel treatment methods and adhesive materials is essential for bonding to PEEK.

Previous studies have explored surface modification techniques for PEEK [13]. Plasma treatment is regarded as an effective method for surface modification [14,15]. Plasma is a partially ionized gas containing electrons, ions, and reactive neutral species, and it is widely employed for modifying polymer surfaces without altering bulk properties. Among the various plasma systems, low-pressure plasma offers a highly controlled environment with reduced collision frequency, enabling the generation and uniform distribution of reactive species while minimizing thermal stress on the substrate. Owing to these characteristics, low-pressure plasma has been used extensively for the surface activation of high-performance polymers such as PEEK [16]. Under low-pressure conditions, reactive oxygen-based species interact with the polymer surface, leading to the degradation and removal of organic contaminants and the introduction of hydrophilic functional groups such as hydroxyl and carboxyl groups. These chemical alterations increase surface free energy and wettability, thereby creating favorable conditions for adhesive bonding [17]. Bötel et al. [18] reported that the PEEK surfaces were treated with low-pressure plasma under an oxygen atmosphere, improving hydrophilicity and bond strength.

In addition to plasma treatment, bonding performance is also strongly influenced by the choice of adhesive system. Chemically polymerized methyl methacrylate (MMA)-based adhesives have been reported to outperform light-cured formulations in terms of bond strength [19], and further improvement has been observed when these adhesives are applied in combination with prior sandblasting of the PEEK surface [20]. However, there is limited systematic evidence on the combined effects of low-pressure plasma treatment and MMA-based adhesives on PEEK bonding, particularly regarding bond durability under different curing modes.

Therefore, the aim of this study focused on assessing how low-pressure plasma treatment affects the bonding behavior of PEEK, as well as examining the performance of a novel MMA-based adhesive under both chemical and light curing conditions. The null hypotheses were that (1) low-pressure plasma treatment would not affect the bond strength to PEEK, and (2) there would be no difference in bond strength between curing modes.

Materials and Methods

Materials used

The materials used in this study are listed in Table 1. A PEEK block for CAD-CAM restoration fabrication (Shofu Block PEEK, 12.0 × 14.4 × 18.0 mm, Shofu, Kyoto, Japan), an adhesive (AD, CAD/CAM Resin Adhesive, Shofu) and a dual-cure resin cement (RC, ResiCem EX, Shofu) were employed. The AD adhesive is a MMA-based, light curing adhesive designed for use with PEEK.

Table 1 Materials used in this study

Abb. Materials* Compositions Lot no. Application procedures
PEEK Shofu Block PEEK poly (etheretherketone) 22021601 ―
AD CAD/CAM Resin Adhesive MMA, UDMA, acetone, camphor-quinone, reducing agent, polymerization inhibitor, other additives (chemical polymerization catalyst, etc.) 092201 apply the adhesive for 10 s, air-dry and light cure for 10 s
RC ResiCem EX paste A: S-PRG filler, Bis-GMA, silicate glass, initiators, others
paste B: S-PRG filler, Bis-GMA, silicate glass, initiators, others
092104 mix pastes A and B and light cure for 40 s (10 s each from 4 different directions)

*Manufacturer: Shofu, Kyoto, Japan

Tensile bond strength test

Specimen preparation method for the tensile bond strength (TBS) test was performed mainly according to the protocol described by Okamura et al. [21], with minor adjustments for the present study, as illustrated in Fig. 1. Procedures including PEEK blocks sectioning, surface grinding, and alumina sandblasting with 50 µm alumina particles were performed according to previous studies. In the present study, the specimen thickness was set to 3.0 mm, and sandblasting was performed at 0.3 MPa. After sandblasting, the specimens were ultrasonically cleaned in distilled water for 5 min, followed by 2 min in 98% ethanol and air-dried. The specimens were then divided into the following two groups; non-plasma-treated (PI[−]) group and the plasma-treated (PI[+]) group. The PI(+) group underwent low-pressure plasma treatment using a low-pressure plasma device (PM100, Yamato Scientific, Tokyo, Japan) under an O2 gas flow for 10 min (chamber pressure: 500 Pa, frequency: 100 kHz, power: 100 W). For all specimens, AD adhesive was applied to the PEEK surface for 10 s and air-dried. The specimens were further divided into two subgroups: specimens in the light-cured (LC) were exposed to light for 10 s using a light-emitting diode curing unit (VALO; standard mode; 1,000 mW/cm2; Ultradent, South Jordan, UT, USA), whereas polymerization in the chemically cured (CC). The bonding area was then demarcated by using a double-sided tape with a 4 mm diameter hole. A stainless-steel rod was placed on the treated surface using a RC and light-cured from four directions at a 45° angle for 10 s each (total of 40 s). The bonded assemblies were left at room temperature for 30 min and then stored in water at 37°C for 24 h.

Fig. 1 Experimental procedure of the TBS test

Thermal cycling (TC) was performed at either 0 cycles (TC0) or 5,000 cycles (TC5,000) using a TC device (K178-08, Tokyo Giken, Tokyo, Japan). The temperature ranged between 5°C and 55°C with a dwell time of 30 s per cycle. After TC0 or TC5,000, TBS was measured using a tabletop universal testing machine (AGS-X, SHIMADZU, Kyoto, Japan) at a crosshead speed of 1.0 mm/min (n = 10).

Failure mode analysis

The failure mode analysis of the debonded specimens after the TBS was performed using a scanning electron microscope (SEM, JSM-IT200LV, JEOL, Akishima, Japan) under low-vacuum conditions at ×30 magnification. The fracture surfaces were classified into four categories based on the failure mode: adhesive failure occurred at the AD-PEEK interface (A); mixed failure consisted of adhesive failure at the AD-PEEK interface combined with cohesive failure within RC, with <20% of RC remaining on the bonded surface (B); 20-50% of RC remaining on the bonded surface (C); and >50% of RC remaining on the bonded surface (D) (Fig. 2).

Fig. 2 Illustration of categorization of the failure modes after TBS testing

A: adhesive failure at the AD-PEEK interface. B: mixed failure consisting of adhesive failure at the AD-PEEK interface and <20% RC remaining on the bonded surface. C: mixed failure consisting of adhesive failure at the AD-PEEK interface and 20-50% RC remaining on the bonded surface. D: mixed failure consisting of adhesive failure at the AD-PEEK interface and >50% RC remaining on the bonded surface.

SEM observation at the adhesive interface

For the SEM observation at the adhesive interface of the PI(+)/LC group, the bonded specimens were prepared in the same manner as the TBS testing. They were sectioned perpendicular to the adhesive interface using a low-speed diamond saw to obtain a 1 mm thick specimen, and embedded in epoxy resin (Epoxicure, Buehler, Lake Bluff, IL, USA). After curing, the specimens were polished with silicon carbide paper (SiC, #600, 800, 1000, and 1,200) and diamond pastes (6, 3, 1, and 0.25 µm, High-Press Diamond Paste, Engis Japan, Yokohama, Japan), and ultrasonically cleaned in distilled water for 2 min. The samples were coated with osmium (Neoc-Pro, Vacuum Device, MEIWAFOSIS, Tokyo, Japan) and observed using SEM (15 kV, ×5,000). The thickness of the AD adhesive was measured vertically at three points, namely, the center of the AD-PEEK interface and two points 10 µm from the center. The mean of the three values was considered the representative thickness for one sample. A mean thickness of the AD adhesive was determined from the measurements of five samples.

Measurement of contact angle on the PEEK surface

The specimen preparation for contact angle measurement is illustrated in Fig. 3. The PEEK surface was polished with 1 µm alumina abrasive particles, followed by ultrasonic cleaning in distilled water for 5 min followed by ethanol for 2 min. The specimens were then divided into two groups: non-plasma-treated PI(−) and the plasma-treated PI(+) group. For the PI(+) group, low-pressure plasma treatment was performed for 10 min using the low-pressure plasma treatment device under the same conditions as the adhesion test. Subsequently, the static contact angle on the PEEK surface was measured at room temperature using an automatic contact angle meter (DM-501, Kyowa Interface Science, Niiza, Japan). A 1.0 µL droplet of distilled water was dispensed onto the PEEK surface, and the contact angle of the water droplet was recorded 10 s later (n = 5). Each measurement was taken at a single point in the center of the PEEK surface.

Fig. 3 Experimental procedure of the contact angle measurement

Statistical analysis

Normality and homogeneity of variance were assessed prior to analysis using the Shapiro-Wilk test and Levene’s test. The TBS data did not meet the assumption of normality (Shapiro-Wilk, P < 0.05), and therefore were analyzed using Dunn’s test with Bonferroni correction. The contact angle data satisfied both normality and homogeneity of variance (P > 0.05), and were evaluated using an independent t-test. A significance level of 5% was set for all statistical analyses. The data were analyzed using statistical software (SPSS ver. 27.0 for Windows, IBM, Armonk, NY, USA).

The sample size was calculated based on data from pilot studies using G*Power 3.1.9.7 (Heinrich Heine University, Düsseldorf, Germany). α error = 0.05, 1-type II error = 0.95, mean differences = 5.4, standard deviation (SD) = 1.8 and 3.7 respectively, effect size (Cohen’s d) = 1.8, and the minimum number of specimens = 8. 10 specimens were prepared to compensate for potential loss. For the contact angle measurement, the sample size was also determined in a post hoc analysis based on the obtained mean and standard deviation, yielding an effect size of 27.7 and a minimum requirement of five specimens.

Results

TBS test

The results of the TBS test are shown in Table 2. In the result of TBS value, a statistical analysis revealed a significant interaction between plasma and curing mode (P < 0.05), whereas neither the interactions between plasma and TC nor between curing mode and TC interactions were statistically significant (P > 0.05).

Table 2 TBS of resin cement to PEEK (MPa)

Plasma treatment Curing mode TC0 TC5,000
median IQR median IQR
PI(−) CC 3.91Abc 3.06-5.67 0.07Aa 0.06-0.10
LC 10.96Bab 6.91-13.21 5.93Bb 5.25-9.25
PI(+) CC 3.74Cbc 2.44-4.53 0.06Ca 0.02-0.13
LC 12.57Da 10.58-14.73 7.48Db 7.06-9.50

For the same row, different uppercase superscripts indicate statistically significant differences between TC0 and TC5,000. For the same column, different lowercase superscripts indicate statistically significant differences between the curing mode (CC and LC) (Dunn's test with Bonferroni correction, P < 0.05) (n = 10).

Failure mode analysis

Representative SEM images of the fracture surfaces after the TBS test are shown in Fig. 4. Figure 4A exhibits an adhesive failure mode at the AD-PEEK interface, characterized by the complete absence of adhesive or resin cement remnants on the PEEK surface. Conversely, Fig. 4B reveals a mixed failure mode, with resin cement covering a limited area (<20%), while no residual adhesive was detected. Figure 4C demonstrates a more extensive distribution of resin cement (20-50%), wherein filler particles within the resin cement matrix are visible. Differences in the failure mode distributions of the debonded specimens were observed among the experimental groups (Table 3 and Fig. 5). In the PI(−)/CC group, mode A predominated over mode B regardless of TC. In the PI(−)/LC group, mode B was more prevalent than mode C in both TC0 and TC5,000. In the PI(+)/CC group, mode A predominated in TC0, whereas mode B was more frequent in TC5,000. In the PI(+)/LC group, mode C predominated in TC0, while mode B was most prevalent in TC5,000, followed by mode C and one mode A specimen.

Fig. 4 Representative SEM images of the failure specimens after TBS test

RC: resin cement; PEEK: poly (etheretherketone). A: adhesive failure at the AD-PEEK interface. B: mixed failure consisting of adhesive failure at the AD-PEEK interface and <20% RC remaining on the bonded surface. C: mixed failure consisting of adhesive failure at the AD-PEEK interface and 20-50% RC remaining on the bonded surface

Table 3 Failure mode analysis of the debonded specimens after TBS test

Plasma treatment Curing mode TC0 TC5,000
PI(−) CC 8/2/0/0 9/1/0/0
LC 0/7/3/0 0/8/2/0
PI(+) CC 6/4/0/0 4/6/0/0
LC 0/3/7/0 1/6/3/0

A/B/C/D, A: adhesive failure at the AD-PEEK interface, B: mixed failure consisting of adhesive failure at the AD-PEEK interface and <20% RC remaining on the bonded surface. C: mixed failure consisting of adhesive failure at the AD-PEEK interface and 20-50% RC remaining on the bonded surface. D: mixed failure consisting of adhesive failure at the AD-PEEK interface and >50% RC remaining on the bonded surface.

Fig. 5 Failure mode analysis of the debonded specimens after TBS test

A: adhesive failure at the AD-PEEK interface. B: mixed failure consisting of adhesive failure at the AD-PEEK interface and <20% RC remaining on the bonded surface. C: mixed failure consisting of adhesive failure at the AD-PEEK interface and 20-50% RC remaining on the bonded surface. D: mixed failure consisting of adhesive failure at the AD-PEEK interface and >50% RC remaining on the bonded surface.

SEM observation of the adhesive interface

The SEM images of the adhesive interface of the PI(+)/LC group are shown in Fig. 6. Good bonding was observed at the interface between the RC and PEEK by the cured AD adhesive. The mean thickness of the AD layer was 5.1 ± 1.1 µm. Electron dense particles were heterogeneously dispersed throughout the PEEK specimens.

Fig. 6 Representative SEM images of the adhesive interface

RC: resin cement; AD: adhesive; PEEK: poly (etheretherketone)

Contact angle measurement of the PEEK surface

Representative images of the contact angle measurements without/with low-pressure plasma treatment are shown in Fig. 7a and b, and the results are presented in Table 4. Plasma treatment significantly reduced the contact angle of the PEEK surface in the PI(+) group compared with the non-treated PI(−) group (P < 0.05).

Fig. 7 Representative images of contact angle measurements for specimens without plasma treatment (a) and with plasma treatment (b)
Table 4 Contact angle results for PEEK without/with plasma treatment

Plasma treatment Contact angle (°)
PI(−) 75.4 ± 3.2a
PI(+) 4.9 ± 0.6b

Mean ± SD (n = 5). Means followed by the different superscript letters were statistically significantly different (an independent t-test, P < 0.05).

Discussion

This study aimed to evaluate the effects of low-pressure plasma treatment and curing mode on the bonding performance of PEEK. Low-pressure plasma treatment improved surface wettability but did not increase bond strength, whereas curing mode had a clear influence, with light curing producing higher bond strength than chemical curing. These results suggest that adhesion to PEEK is governed more by the efficiency of polymerization than by surface activation alone. Based on these findings, null hypothesis (1) could not be rejected, whereas null hypothesis (2) was rejected.

Due to its chemical stability, PEEK does not respond well to surface treatments using functional monomers typically used for dental materials, and thus reliable adhesion has been difficult to establish [11,12]. To enhance the bonding surface and mechanical interlocking effect, sandblasting was performed on a PEEK surface. Okamura et al. [21] investigated the adhesion effect of CAD-CAM resin blocks treated with a chairside particle abrader and reported that the optimal air pressure for resin blocks was 0.2 MPa. However, there are few reports on the appropriate air pressure for sandblasting PEEK surfaces [22]. In the current study, the air pressure was determined at 0.3 MPa according to a previous study [23].

Low-pressure plasma treatment was applied to modify the PEEK surface in this study. Plasma is a state in which electrons are separated from atoms or molecules by adding energy to gases such as oxygen or argon, creating a mixture of positive ions, electrons, and radicals [24]. When reactive species generated in the plasma phase interact with the material surface, organic contaminants are decomposed and removed, while oxygen-containing functional groups such as hydroxyl (-OH) and carboxyl (-COOH) are introduced. These chemical modifications increase surface polarity and thereby enhance wettability and surface free energy [17]. It was reported that plasma treatment increased the surface polarity of materials, enhancing surface energy, hydrophilicity, and adhesion properties [18,25]. It is well established that improvements in surface wettability and surface free energy reduce the interfacial distance between the substrate and the adhesive, thereby increasing intermolecular forces and enhancing bond strength.

In this study, the effect of low-pressure plasma treatment on the PEEK surface was evaluated by measuring the contact angle. The results demonstrated that low-pressure plasma treatment significantly reduced the contact angle of the PEEK surface. This finding indicates that low-pressure plasma treatment improved the wettability of the PEEK surface, making it more hydrophilic.

Low-pressure oxygen plasma is known to introduce oxygen-containing functional groups, such as hydroxyl and carboxyl groups, onto polymer surfaces, thereby increasing surface polarity and surface free energy [17,18]. These changes facilitate improved spreading and intimate contact of adhesive materials on the treated surface. However, in contrast to a previous study [18], the TBS test results in this study showed no interaction between plasma treatment and TC, and bond strength was not improved. Although plasma treatment significantly improved wettability, the differences from previous findings may be attributed to variations in plasma treatment conditions. The low-pressure plasma treatment parameters used in this study (O2: flow for 10 min, chamber pressure: 500 Pa, frequency: 100 kHz, power: 100 W) were determined based on the maximum stable operating conditions of the device, previous reports, and practical applicability [12,14,18,26,27,28,29]. These parameters were intended to influence surface characteristics while maintaining safe and clinically feasible conditions, and to enable reproducible plasma generation with a balance between effective surface activation and preservation of the bulk properties of the polymer substrate, within the safety specifications of the device. However, such parameters inherently vary across devices due to differences in chamber design and plasma density, and these factors should be considered when comparing results among studies [27,30].

This discrepancy may be attributed not only to differences in the type of gas and treatment duration, but also to variations in plasma device settings, surface characterization methods, and possible differences in the storage conditions of specimens. These factors highlight the need for standardized protocols for plasma treatment of PEEK surfaces in future studies. Plasma-induced oxygen-containing functional groups may diminish over time because of hydrophobic recovery, resulting in a gradual decrease in wettability. This temporal change may further account for the lack of improvement in bond strength.

The AD adhesive is MMA-based and contains camphorquinone as the photo-initiator. Previous studies [17,24,31] have reported the effectiveness of MMA-containing resin-based materials for bonding to PEEK. MMA has the lowest molecular weight among the monomers used for the dental materials, allowing it to penetrate into the polymer network of the PEEK substrate, thereby enhancing adhesion. Although low-pressure plasma treatment significantly improved surface wettability, no interaction between plasma treatment and TC, and bond strength was not improved. This lack of statistical significance may be attributable to the limited contribution of surface activation alone when using an MMA-based adhesive system, as well as to variability in bond strength measurements under the present experimental conditions. However, a statistically significant interaction was detected between plasma treatment and curing mode. Light polymerization is generally considered to achieve a higher degree of conversion than chemical polymerization [32]. In addition, photopolymerization of multifunctional monomers proceeds rapidly, leading to the formation of a highly cross-linked polymer network [33]. In light of the present results, these factors may have promoted and stabilized the polymerization of MMA that had slightly penetrated the PEEK surface, thereby contributing to the enhanced bond strength observed under light curing conditions. Conversely, under chemical curing conditions, the relatively slower and less complete curing process may have been insufficient to effectively stabilize the MMA-PEEK interface, potentially resulting in the reduced bond strength following plasma treatment.

In this study, the bonding durability was evaluated by using a TC test. Generally, bonding between two materials with different coefficients of thermal expansion causes stresses at the adhesive interface between two materials during TC, resulting in water infiltration at the adhesive interface, and reducing bond durability [34,35]. It has been reported that chemically polymerized resin cements exhibit reduced bond strength after TC, compared with their initial adhesion [32]. This phenomenon is thought to be attributable to the time-dependent degree of conversion as well as the influence of post-polymerization cross-linking structures on bond strength. However, no significant interaction was observed between plasma treatment and TC, nor between curing mode and TC. Also, in all the groups except the PI(+)/LC group, adhesive failure occurred at the AD-PEEK interface or mode B mixed failure (<20% RC) was predominantly observed, with no changes in the failure mode distribution before and after TC. However, a significant interaction between plasma treatment and curing mode was observed. Also, the PI(+)/LC group showed high frequency of mode C mixed failure (20-50% RC) and also no adhesive failure was observed in TC0. Whereas adhesive failure was detected and mode B mixed failure (<20% RC) increased in TC5,000. The observed changes suggest a potential influence of plasma treatment and chemical curing mode.

Due to its mechanical properties, PEEK is expected to be a viable option for metal-free restorations in posterior teeth. From the results of the current study, it was suggested that light curing of the AD adhesive may be necessary to achieve reliable bonding to PEEK.

Low-pressure plasma treatment did not result in a significant increase in bond strength; however, it improved surface wettability and was suggested to influence the fracture surface morphology. These findings indicate that surface activation by low-pressure plasma alone is insufficient to achieve reliable adhesion to PEEK under the conditions tested. Nevertheless, the present study was limited to a single plasma device, adhesive formulation, and bonding protocol. Future studies should explore standardized plasma parameters, the stability of plasma-induced functional groups over time, and the synergistic effects of combining plasma treatment with chemically tailored adhesive systems. Further research should be performed to evaluate the optimal air pressure for treating a PEEK surface.

Abbreviations

Abb.: abbreviation, AD: CAD/CAM Resin Adhesive, Al2O3: aluminum oxide, Bis-GMA: bisphenol a glycidyl methacrylate, CAD-CAM: computer-aided design and computer-aided manufacturing, CC: chemically cured, e-: electron, IQR: interquartile range, LC: light-cured, MMA: methyl methacrylate, PEEK: poly (etheretherketone), PI(+): plasma-treated, PI(−): non-plasma-treated, O2: oxygen, O2-: oxide ion, RC: ResiCem EX, S-PRG: surface pre-reacted glass ionomer, SD: standard deviation, SEM: scanning electron microscope, SiC: silicon carbide, TBS: tensile bond strength, TC: thermal cycling, UDMA: urethane dimethacrylate

Ethical Statements

This study involved only in vitro experiments and did not include human or animal subjects.

Conflicts of Interest

Not applicable

Funding

Not applicable

Author Contributions

RI: conceptualization, data curation, formal analysis, investigation, methodology, visualization, and writing; SS: conceptualization, data curation, formal analysis, methodology, project administration, supervision, writing, review, and editing; MU: conceptualization, formal analysis, methodology, resources, supervision, writing, review, and editing; HT: investigation, data curation; MI: formal analysis, methodology, supervision, review, and editing; MB: formal analysis, writing, review and editing; TN: conceptualization, formal analysis, methodology, writing, review, editing, and supervision; KO: conceptualization, formal analysis, methodology, writing, review, editing, and supervision. All authors read and approved the final version of the manuscript.

ORCID iD

  • 1) RI: ito-rikari@asahi-u.ac.jp, https://orcid.org/0009-0006-1758-4382

    1) SS*: shojiro0914@asahi-u.ac.jp, https://orcid.org/0009-0000-6572-5537

    2) MU: uo.abm@tmd.ac.jp, https://orcid.org/0000-0002-0292-2127

    1) HT: karubonala@asahi-u.ac.jp, https://orcid.org/0009-0005-3511-1493

    3) MI: ikedsdt@tmd.ac.jp, https://orcid.org/0000-0003-2214-4980

    4) MB: mfburr58@hku.hk, https://orcid.org/0000-0001-6419-6530

    5) TN: nikaido-ope@asahi-u.ac.jp, https://orcid.org/0000-0002-7346-1831

    1) KO: katsu@asahi-u.ac.jp, https://orcid.org/0000-0002-0062-5495

Acknowledgments

The contact angle measurement was supported by Prof. Akira Matsumoto, Department of Organic Biomaterials, Laboratory for Biomaterials and Bioengineering, Institute of Science Tokyo.

Data Availability Statements

All data generated or analyzed during the current study are available from the corresponding author on reasonable request.

References
 
© 2026 Japanese Dental Science Federation

This article is licensed under a Creative Commons [Attribution-NonCommercial-NoDerivatives 4.0 International] license.
https://creativecommons.org/licenses/by-nc-nd/4.0/
feedback
Top