The trend toward multi–material industrial products is advancing to achieve goals like carbon neutrality. Joining technologies between dissimilar metallic materials are essential for this multi–materialization. However, dissimilar metallic materials exhibit differing physical properties such as melting points, thermal expansion coefficients, and thermal conductivity coefficients.
While brazing is considered suitable for joining dissimilar metallic materials, creating a sound interface through brazing between them is known to be difficult.
Previous research indicates that precisely controlling the amount of molten brazing filler metal during brazing is difficult. Although research continues, no solution has yet been demonstrated.
Therefore, this study proposes a method where the base metal is rotated during brazing to forcibly expel molten filler metal outside the brazed joint.
Reducing the amount of brazing filler metals often leads to a reduction in the thickness of the brazing zone. A thinner brazing zone can increase the strength of the brazed joint. Furthermore, we believe that expelling the molten brazing material outward can suppress the formation of intermetallic compounds and other phases at the interface.
The base materials used were free–cutting brass and austenitic stainless steel SUS304L. The brazing filler metal used was BAg–7, a foil–type silver–based brazing filler metal. Brazing was performed in a vertical electric furnace. The brazing temperature was approximately 700°C, with a brazing hold time of 5 minutes. Rotation was applied at 100 rpm.
For brazing evaluation, microstructural observation was performed using an optical microscope, and mapping elemental analysis was conducted using EPMA for analysis.
View full abstract