  • 渡辺 正紀, 蒲地 一義
    1961 年30 巻6 号 p. 376-386
    発行日: 1961/06/25
    公開日: 2011/08/05
    ジャーナル フリー
  • 多田 美朝, 立花 一郎, 寺尾 貞一
    1961 年30 巻6 号 p. 387-393
    発行日: 1961/06/25
    公開日: 2011/08/05
    ジャーナル フリー
    Occurrence of undercutting in welded joint is inevitable in some welding position such as horizontal, verticul or overhead. Undercutting, must affect the fatigue strength of welded joint as it constitutes a notch. From this standpoint, the relation between the undercut depth and the fatigue strength was experimentally studied on the test pieces, which were taken from butt welded joints and fillet welded plates of mild steel.
    Test pieces were prepared according to Fig. 2 in the shape as shown by Fig. 1 ; types and undercut depths of test pieces are listed in Table 2. The undercut depth was measured using the instrument shown in Fig. 3. Fatigue tests were conducted under pulsating tension. The testing machine was a 20t capacity hydraulic type. The tests were carried out up to 5 × 106 cycles. Understandably, the failure originated at the root of undercut in all test pieces.
    The results of fatigue tests are shown in Figs. 5 and 6, and the 2 × 106 fatigue strength value (range of stress), obtained through interpolation and extrapolation, were plotted on a probability paper (Figs. 7 and 8). Then the mean value and the values of 5% probability and 95% probability of failure were plotted against the undercut depth in Figs. 9 and 10. Considerable variances are observed in the S-N curves of Figs. 5 and 6. These variances are represented by the fattened portions of vertical lines in Figs. 9 and 10; they are particularly wide in the case of the butt welded joint with a 0 mm undercut depth, and in that of -the fillet welded plate with a 0.5 mm undercut depth. Perhaps it so seems on account of the number of test pieces being limited.
    As seen from Fig. 9, the fatigue strength decreases in butt welded joints with an increase in the undercut depth ; namely, it is seriously influenced by the undercut depth. By contrast, it is some what less influenced in the case of fillet welded plate, but ceases to decline beyond 0.3 mm. Perhaps there exists already a stress concentration at the toe of fillet and the notch effect in this area must be mitigated. It is due to an imperfect machining that no improvement on fatigue strength was observed in the machined test piece with a 0.46 mm undercut.
  • 珪素脱酸における炭素の影響
    榊 鳳千代
    1961 年30 巻6 号 p. 394-397
    発行日: 1961/06/25
    公開日: 2011/08/05
    ジャーナル フリー
    In ordinary manual arc welding, the weld metals was obtained by successive addition of graphite from lime-fluorides type flux. The effect of carbon on Charpy V-noth properties was determined on the weld metals thus obtained.
    Carbon fines ferrite grain size of weld metals, reduces maximum energy rapidly, increases transition temperature at a rate of 15°C per 0.1%, and widens transition range regularly.
  • 鈴木 春義, 田村 博, 小林 卓也
    1961 年30 巻6 号 p. 398-406
    発行日: 1961/06/25
    公開日: 2011/08/05
    ジャーナル フリー
    Correlation between weld HAZ ductility and hardness were conducted for twelve high strength steels by means of a Kommerell bead-bend test. The critical values of HAZ hardness at which HAZ ductility becomes unsatisfactory were determined for each steel. These values differ not a little from steel to steel, and were concluded to be very important as a criterion of survice performance of high strength steel weldments. Furthermore, these critical values were found to be closely related to those obtained from "the synthetic HAZ ductility test" newly introduced by authors.
  • 安藤 精一, 森 三郎
    1961 年30 巻6 号 p. 407-417
    発行日: 1961/06/25
    公開日: 2011/08/05
    ジャーナル フリー
    Authors surveyed the influences of three different methods (JIS, modified ISO and ISO) for the tensile test of deposited metal-in the former two, in as welded condition and in the latter, after hydrogen removing treatment, the test is carried out-upon fisheye appearances and mechanical properties of deposited metals from various types of mild steel electrodes, and further investigated some metal-lurgical properties of deposited metals.
    From the experimental results, authors found that fisheye appearances revealed in ordinary strain rate at room temperature are influenced by the deoxidation degree, the diffussible hydrogen content existing in time of test, the size and number of porosities in deposited metal.
  • 鈴木 春義, 橋本 達哉, 松田 福久, 田沼 欣司
    1961 年30 巻6 号 p. 418-428
    発行日: 1961/06/25
    公開日: 2011/08/05
    ジャーナル フリー
    ZrおよびZr-2を空気中でスポット溶接し,その溶接適正条件と溶接継手の機械的ならびに高温水中の腐食試験による性能試験をおこなった.その結果つぎの結論をえた.
    (1)溶接前の表面処理はペーパ処理または化学酸洗(HF 5%+HNO3 45%+H2O 50%,20秒)がよい.しかし処理精度の均一性,電極の消耗,および原子炉中の腐食の点よりみて化学酸洗のほうがより望ましいと考えられる.
    (2)本実験の範囲内では適正なスポット溶接条件として近似的に次式のような実験式がえられた.
    電流(I)=5000+5000T0 (A)
    圧力(P)=80+220T0 (kg)
    通電時間(t)=1+5T0 (Cycles)
    ただしT0=溶接板の板厚(mm)
    (3)スポット溶接部には気泡,割れその他の欠陥は全く認められなかった.
    (4)適正溶接条件でおこなったスポット溶接部の機械的性質について次のことがいえる.
    (i)引張せん断試験では,破断は熱影響部と素材の間でおこり,ボタン状の破断を示す.
    (ii)引張せん断強さは板厚と共に増加し,実験範囲内では板厚1mmの増加にともないZrでは約700~800kg,Zr-2では1,000~1,500kg程度増加する.またZr-2はZrに比し強さが大である.焼なまし後の強さは焼なまし温度が上昇するにしたがい急速に低下していく.
    (iii)ナゲット部のかたさはTIG溶接部に比しかなり高い.この原因は空気中の酸素,窒素ガスの吸収によるものではなく冷却速度が速いための焼入硬化に起因する.
    (iv)ナゲット部の組織は巨大な樹枝状晶を示し,各樹枝状晶内はほとんど完全なα'(acicular α)であり,硬化もこのα'に起因しているものと思われる.
    (5)適正溶接条件と溶接部の機械的性質を総合してZrおよびZr-2の点溶接の作業基準を求めるとTable 4がえられる.
    (6)溶接部近傍の熱サイクルの測定結果によれば,空気と接触する部分が400~500℃以上の高温に保たれる時間は数サイクル~10サイクル程度である。したがってこの時間内に空気中の酸素,窒素ガスが素材と反応する程度はごくわずかで,その悪影響は無視できるほどである.
    (7)溶接継手の高温高圧水(320℃,115~117気圧)に対する耐食性は溶接後の酸洗の有無にかかわらず健全である.
    以上の実験結果よりZrおよびZr-2を空気中でスポット溶接した継手は化学工業用にはもちろん原子炉用としても何ら懸念することなく使用できる.
    最後に本研究に対し,高温高圧水の腐食に関して金属材料技術研究所第五部の伊藤博士と清水技官の絶大な御指導,御協力をいただいた.また材料は日本金属工業(株)の御厚意によるものでありここに厚く感謝の意を表する。
  • 伊藤 慶典
    1961 年30 巻6 号 p. 429-434
    発行日: 1961/06/25
    公開日: 2011/08/05
    ジャーナル フリー
    The crack sensitivity and the strength at high temperature of type 347 Cr-Ni austenitic weld metal with 3.5-8.5% Mn made by Argon-arc or coated metal arc welding, are researched. The ex-perimental results are as follows.
    (1) Addition of Mn to type 347 weld metal decreases crack sensitivity.
    (2) In the case of fully austenitic weld metal made by the suitable addition of Mn, Sigma phase can not be formed under high temperature for 1, 000 hours.
    (3) The creep rupture strength at 650°C of fully austenitic weld metal with suitable additional Mn, is superior to the standard type 347 weld metal.