Abstract
The experiment has been carriedto find the actual strength of glass plate which used as a building materials. This report consisted from following.
1. To find the uniform load using the samples which having different thickness and area.
2. To calculate the bending strength from above exp. and obtained the result as following.
730 kg/cm2 for 2mm. thickness.
560kg/cm2 for 3mm. thickness.
470kg/cm2 for 5mm. thickness.
420kg/cm2 for 6mm. thickness.
3. To calculate the hydrauric and wind pressure and then compared to the uniform load which obtaind by above experiment.