Abstract
Cs0.9Al0.9Si2.1O6 is an aluminosilicate compound showing a low thermal expansion property. In this work, the porous body of Cs0.9Al0.9Si2.1O6 was fabricated by an addition of PMMA. When 40wt% PMMA was added, the porous body fabricated by a heat treatment of 1400°C for 20h, had the relative density of 46% and showed the thermal expansion rate of 0.105% with a small hysteresis. Thus it was found that the porous body of Cs0.9Al0.9Si2.1O6 showed a further low-thermal expansion property.