The diamond photonic crystals with periodic arrangement of dielectric media were fabricated, and millimeter wave localization behaviors in introduced structure defects introduced were investigated. Acrylic diamond lattice structures with TiO2 dispersion at 40 vol. % were fabricated by Microstereolithography. After removing acrylic resin by heating in air at 600 deg C for 2 hours, the sample was sintered at 1350 deg C for 2 hours. The electromagnetic properties of sintered samples were measured with network analyzer and W-band millimeter waveguide in the range from 75 GHz to 110 GHz. The behavior of the defect mode will be reported.