Abstract
Solubilities of nitrogen in liquid Fe-Ti, Fe-V, Fe-Cr, Fe-Mo, and Fe-W alloys are determined in the temperature range of 1580°C to 1 680°C by sampling method.
The results obtained show that addition of Ti, V, Cr, Mo, and W increases the solubility of nitrogen in liquid iron. The effects of alloying elements on the activity of nitrogen in liquid iron at 1 580° are expressed as follows:
logf TiN=-0.9 [%Ti] <0.15%Ti, PN2=0.040.17atm logf VN=-0.10 [%V] <6.5%V