2021 Volume 27 Issue 65 Pages 18-23
This study optimized the binder composition for making 300N/mm2 ultra-high-strength concrete. The use of silica fume with a replacement ratio of 24%, which contained 50% coarse silica flour, attained both high compressive strength and high fluidity. The newly developed chemical admixture showed excellent dispersibility down to 10% water-to-binder ratio, which improved concrete workability, mitigated the delayed setting times, and resulted in 30% less shrinkage and 7% strength gain. For the design strength of 300N/mm2, satisfactory strength and workability can be reached with the specific aggregates and curing scheme reported in our previous study.
Ethical standards of the publisher (‘Ethical Standards Concerning the Peer Review for the Presentation of Architectural Transactions and Works’)