材料試験
Print ISSN : 0372-7971
鋼の焼なまし時における応力弛緩に対する前熱処理の影響
伊藤 篤
著者情報
ジャーナル フリー

1962 年 11 巻 107 号 p. 499-503

詳細
抄録
Effects of pre-heattreatment on the anisothermal relaxation of S30C, S45C, SUP3 and quasi-SUP6 during annealing were studied.
In order to investigate the relaxation behavior, the changes of load of variously heat-treated steels, which were made to keep the constant deflection in the 4-points-support bending tests, were measured continuously during heating and cooling. In annealed steel, the load remained, to some extent, upto temperature Ac1, but in quenched or quenched and tempered steel, a sharp decrease of the load was recognized with progress of tempering process. These phenomena can be explained by considering the high-deformability of steel during its structural change. It is necessary to consider these facts in the discussion of the mechanism of stress-relief-annealing.
著者関連情報
© 日本材料学会
前の記事 次の記事
feedback
Top