地下水使用環境下での銅管の孔食
山田 豊河野 浩三鈴木 忍渥美 哲郎
著者情報
ジャーナル フリー

1999 年 48 巻 10 号 p. 647-653

詳細
抄録
Pitting corrosion of copper soft tubes has been experienced in the pass-through plumbing system using well water. Although the morphology of the pitting was similar to type 1 pitting corrosion of copper tubes, the quality of well water was different from those in plumbing system. The factor of the pitting corrosion has been investigated by field test in actual plumbing system. The free carbon dioxide in well water was 17 to 20ppm. The presence of both carbon film on the copper tubes and free carbon dioxide in well water caused the pitting corrosion. The pitting corrosion of copper tubes occurred under the presence of both residual ferr carbon more than 5mg/m2 and free carbon dioxide more than 15ppm.