鉄と鋼
Online ISSN : 1883-2954
Print ISSN : 0021-1575
ISSN-L : 0021-1575
論文
高温性状試験における鉱石層厚の還元率と圧力損失に及ぼす影響の評価
西村 恒久樋口 謙一大野 光一郎国友 和也
著者情報
ジャーナル オープンアクセス HTML

2016 年 102 巻 2 号 p. 61-67

詳細
抄録
To evaluate condition and distribution of reduction degree and gas permeability in ore layer, examinations of high temperature properties with various ore layer thickness were executed. Gas permeability begins to decrease from the upper part of ore layer, where melt with more FeO is formed with low reduction degree. Experimental results show that the difference of reduction degree in ore layer of examination of high temperature properties is about 40% at 1200°C. Estimation with mathematical model indicates that difference of reduction degree in ore layer increases with decreasing gas flow rate.
著者関連情報
© 2016 一般社団法人 日本鉄鋼協会

This article is licensed under a Creative Commons [Attribution-NonCommercial-NoDerivatives 4.0 International] license.
https://creativecommons.org/licenses/by-nc-nd/4.0/
次の記事
feedback
Top