周方向表面欠陥を有する 6inch口径ステンレス鋼製配管の不安定破壊試験
植田 修三, 栗原 良一, 加藤 潔, 鬼沢 邦雄, 関谷 秀郎, 宮園 昭八郎
著者情報
ジャーナル フリー

1987 年 53 巻 495 号 p. 2097-2100

詳細
抄録
The authors are performing an unstable fracture test of circumferentially cracked pipes in order to investigate the possibility of mitigating the conservative assumption of guillotine break in light-water reactor pressure boundary piping. The tests were performed at 285°C and at 6.86 MPa using type 304 stainless steel pipes of 165.2 mm in diameter and 11.0 mm in thickness. It is concluded that the predicted fracture load by the net-section-stress approach is conservative in a limited range of crack dimensions.